SAF Duplex 2205 Stainless Steel (UNS S32205 S31803) Alloy Material Data Sheet, Properties, Composition, Density (2024)

SAF Duplex 2205 Stainless Steel (UNS S32205 S31803) Alloy Material

SAF Duplex 2205 stainless steel (UNS S32205 formerly known as UNS S31803 and commonly known as “alloy 2205”) has a mixed microstructure of austenite and ferrite, and is a two-phase alloy based on the Fe-Cr-Ni series. Alloy 2205 material has lower nickel and molybdenum contents than austenitic stainless steel and have similar corrosion resistance. Because the price of Ni and Mo is relatively high, duplex stainless steel 2205 is often regarded as a cost-effective alternative to austenitic stainless steel.

Compared with the conventional 300 series stainless steel (e.g. SS 304, SS 316, SS 301, SS 904L, and 303, etc.), the special advantages of duplex 2205 stainless steel are strength (about twice that of austenitic stainless steel), and excellent resistance to chloride SCC and pitting corrosion. High yield strength has sufficient pressure and load capacity, and thin-wall materials can be made to greatly reduce weight.

Duplex 2205 Data Sheet & Specification

The following tables show SAF 2205 duplex stainless steel datasheet and specifications, such as chemical composition, physical properties, mechanical properties, heat treatment, welding, etc.

Chemical Composition

The following table lists alloy 2205 stainless steel chemical composition based on cast analysis.

Chemical Composition, %
CountrySteel Grade (UNS)StandardC, ≤Si, ≤Mn, ≤P, ≤S, ≤CrNiMoN
US2205 (UNS S32205, UNS S31803)ASTM A276/A276M; ASTM A240/A240M0,0301,002,000,0300,02022.0-23.04,5-6,53.0-3.50.14-0.20

Physical Properties

Notes:

  • 1 g/cm3 = 1 kg/dm3 = 1000 kg/m3;
  • 1 μΩ·m = 1 Ω·mm²/m
  • 1 GPa = 1 kN/mm2
Physical Properties
Density, g/cm3 (lb/in3)7,83 (0.283)
Melting point, ℃ (°F)1385-1440 (2525-2630)
MagneticYes
Electrical resistivity, μΩ·m0,85 (20 ℃) (68 °F)
0,90 (100 ℃) (212 °F)
0,95 (200 ℃) (392 °F)
1,0 (300 ℃) (572 °F)
Specific heat capacity, J/(kg·K)470 (20 ℃) (68 °F)
500 (100 ℃) (212 °F)
530 (200 ℃) (392 °F)
560 (300 ℃) (572 °F)
Thermal conductivity, (W/m·K)15,0 (20 ℃) (68 °F)
15,9 (100 ℃) (212 °F)
17,0 (200 ℃) (392 °F)
18,0 (300 ℃) (572 °F)
Modulus of elasticity, Gpa190 (20 ℃) (68 °F)
180 (100 ℃) (212 °F)
175 (200 ℃) (392 °F)
171 (300 ℃) (572 °F)
Mean coefficient of thermal expansion, (10-6/K)13,5 (20-100 ℃) (68 °F – 212 °F)
14.0 (20-200 ℃) (68 °F – 392 °F)
14.6 (20-300 ℃) (68 °F – 572 °F)

Mechanical Properties

Duplex 2205 stainless steel mechanical properties at room temperature in various conditions and resistance to intergranular corrosion, including yield strength, tensile strength, and hardness, etc.

Mechanical properties
Country (Region)StandardAISI Type (UNS)0.2% proof strength, MPa (ksi), ≥Tensile strength, MPa (ksi), ≥Elongation in 50mm (2 in.), %, ≥Brinell Hardness (HBW), ≤Rockwell Hardness (HRC), ≥Condition & Finish
USASTM A276/A276M2205 (UNS S32205, UNS S31803)450 (65)655 (95)25290Annealed, hot-finished or cold-finished
ASTM A240/A240M450 (65)655 (95)2529331

SAF Duplex 2205 Stainless Steel Heat Treatment

Recommended annealing temperature for duplex 2205 stainless steel is 1040 ℃ (1900 °F), cooling from the annealing temperature must be rapid, water quenching is preferred, but it must also meet the limits of deformation. This treatment is suitable for full solution annealing and stress relief annealing.

Hot Forming

Alloy 2205 material hot forming temperature range is 1200-955 °C (2190-1750°F). It is recommended to perform a full annealing with rapid cooling after hot forming, preferably water quenching.

Cold Forming

Due to its higher strength, the force required for cold forming of alloy SAF 2205 is greater than the typical force of austenitic stainless steel. Full annealing and quenching are recommended after severe cold forming.

Welding

SS 2205 duplex can be welded by all common welding processes (except gas welding), such as MMA/SMAW, MIG/GMAW, TIG/GTAW, FCAW, SAW and PAW, and can be welded to carbon steels, low alloy steels or austenitic stainless steels, filler metal can be duplex, super duplex, E2209, E2594, 309L or 309LMo.

  • The maximum interpass temperature is 150°C (300°F),
  • Preheating is not necessary,
  • and postweld heat treatment is not recommended, if necessary, should be done at 1040°C (1900°F) minimum, followed by rapid cooling.

Machining

The high strength makes SAF 2205 stainless steel difficult to machine and therefore requires powerful machines and very strong tool supports. Cutting speed should be reduced by about 20% than the typical type 316L Cutting speed.

Corrosion Resistance

Alloy 2205 (UNS S31803, S32205) has much better corrosion resistance than stainless steel 304 and SS 316, such as excellent pitting resistance (PREN = 30.5), superior resistance to chloride SCC, and resistance to abrasion.

Heat Resistance

The maximum temperature for duplex 2205 stainless steel applications is generally below 300 °C (570 °F), because the high alloy content and the presence of a ferrite matrix make it susceptible to embrittlement and reduced mechanical strength, especially toughness, due to prolonged exposure to high temperatures.

Uses and Applications

Duplex 2205 stainless steel has been widely used in many industries, especially the oil and gas, petrochemical and pulp and paper industries. They are typically used in aqueous, chloride-containing environments and as a substitute for austenitic stainless steels, which are subject to chloride SCC or pitting during use.

SAF Duplex 2205 Equivalent Grade

SAF Duplex 2205 stainless steel (UNS S32205, formerly UNS S31803) equivalent to ASTM AISI SAE, ISO, European (German DIN, British BSI, France NF), Japanese JIS and Chinese GB standard (for reference).

Duplex 2205 equivalent grade
USEuropean UnionISOChinaJapan
StandardGrade (UNS)StandardSteel Name (Material Number)StandardGrade (ISO number )StandardGrade (UNS)StandardGrade
AISI;
ASTM A240/A240M;
ASTM A276/A276M;
Duplex 2205 (UNS S32205); UNS S31803EN 10088-2;
EN 10088-3
X2CrNiMoN22-5-3 (1.4462)ISO 15510X2CrNiMoN22-5-3 (4462-318-03-I)GB/T 1220;
GB/T 3280
022Cr22Ni5Mo3N (S22293)JIS G4303; JIS G4304; JIS G4305SUS329J3L
SAF Duplex 2205 Stainless Steel (UNS S32205 S31803) Alloy Material Data Sheet, Properties, Composition, Density (2024)

References

Top Articles
Latest Posts
Article information

Author: Cheryll Lueilwitz

Last Updated:

Views: 5740

Rating: 4.3 / 5 (74 voted)

Reviews: 89% of readers found this page helpful

Author information

Name: Cheryll Lueilwitz

Birthday: 1997-12-23

Address: 4653 O'Kon Hill, Lake Juanstad, AR 65469

Phone: +494124489301

Job: Marketing Representative

Hobby: Reading, Ice skating, Foraging, BASE jumping, Hiking, Skateboarding, Kayaking

Introduction: My name is Cheryll Lueilwitz, I am a sparkling, clean, super, lucky, joyous, outstanding, lucky person who loves writing and wants to share my knowledge and understanding with you.